FeCrAl fiber-reinforced hydroxyapatite(HA) biocomposites(FeCrAl(f)/HA) were fabricated by the hot pressing technique.The metallographic microscopy,X-ray diffractometry,scanning electron microscopy(SEM) and energy dispersive spectroscopy(EDS) were used to observe and analyze the microstructure and composition of FeCrAl(f)/HA composites,respectively.The mechanical properties of FeCrAl(f)/HA composites were measured by the three-point-bending test.The results show that the composite can be reinforced by FeCrAl fiber and enhanced gradually,and then declined with the increase of the content of FeCrAl fiber(0-11%,volume fraction) in the whole range of experiments.Both the HA matrix and FeCrAl fiber integrate very tightly and bit into each other very deeply and counter-diffusion takes place to some extent at two-phase interface.The optimum parameters of FeCrAl(f)/HA composite are diameter of 22 μm,length of 1-2 mm and of volume faction of about 7% for FeCrAl fibers.